This work aims to identify common challenges in the preparation of the
blister test devices designed for measurement of energy release rate for
brittle thin films and to propose easy-to-implement solutions accordingly. To
this end, we provide a step-by-step guide for fabricating a blister test device
comprised of thin polystyrene films adhered to glass substrates. Thin films are
first transferred from donor substrates to an air-water interface, which is
then used as a platform to locate them on a receiver substrate. We embed a
microchannel at the back of the device to evacuate the air trapped in the
opening, through which the pressure is applied. We quantify the height and the
radius of the blister to estimate the adhesion energy using the available
expressions correlating the normal force and the moment with the shape of the
blister. The present blister test provided adhesion energy per unit area of G=18±2 \mbox{mJ}/{\mbox m}^2 for polystyrene on glass, which is in good
agreement with the measurement of G=14±2 \mbox{mJ}/{\mbox m}^2 found
in our independent cleavage test