Abstract
In continuation of the foregoing paper,the present one deals with the next step of
treatments in the “Presiton Process" on a semi industrial scale for the present sample,
‘Presiton S'. which is to bring about a thin outer layer of the second resin on the surface
of the sample,and also to set the reactive dye at the same time on the peeled
and disc10sed surface of the cellulosic fiber.
The meaning and the theory of preparing ‘Presiton SW' are herewith given in the
introduction. And the optimum conditions of preparing a good ‘Presiton SW' with respect
to the used resin and dye are determined. and given as in the followings;
The reactive dye ; Procion Brill. Orange GS
The dye concentration in the 1st bath; 1 %
The dip time 15 minutes
The resin COnc. in the 2nd bath ; 4 %
Catalyser ;D.A.P.,5 %, o. w. of resin
Cure temp. and time ; 130℃ x 5 min