The Effect of ODC-Free Cleaning Techniques on Bearing Lifetimes in the Parched Elastohydrodynamic Regime

Abstract

A parched elastohydrodynamic rig was used to determine relative bearing lifetimes as a function of cleaning procedures in a series of accelerated tests. Two ODC-free cleaning procedures (super critical CO2 and ultraviolet-ozone) were compared to a CFC-113 control. Bearings (52100 steel) were run in the counter rotating mode (equivalent to 4600 rpm) with a full complement (i.e. no retainer) and a single charge of lubricant (Krytox 143 AC). Test conditions included: an air atmosphere, 445 N load, approx. 1.0 GPa mean Hertz stress. There was approximately a 50% reduction in life with bearings cleaned with UV/ozone and a 70% reduction in life with SFE CO2 when compared to the Freon control. Possible reasons for these decreases in lifetimes are presented