Сибирский федеральный университет. Siberian Federal University.
Abstract
The influence of alkaline activation on the development of anthracite porous structure under the
variation of different factors: anthracite and metal hydroxide origin, their mass ratio in a mixture,
activation temperature and duration has been studied. The highest development of anthracite surface
area was reached with mass ratio of anthracite/alkali 1:5-7 and the final heating temperature of 800 °С.
Under these conditions the maximum value of surface area of carbon material was 2900 m2/g in case of
КОН activated Siberian anthracite and 2550 m2/g for NaOH activated Ilovaisky anthracite