Small Heat Exchanger ORNL #1, type SHE #2, was removed form test stand B after 2071 hours of operation. Thirty-five samples were removed form the entire heat exchanger. The corrosion found on the outside of the tubes exposed to the fluoride mixture ranged to a maximum depth of .004 inches; however, the frequency of occurrence along the tube wall was heavier at the NaK outlet header, which was the hottest area in the heat exchanger. The depth of attack observed on the fluoride side of this heat exchanger was uniform from header to header and did not exceed .004 inches