Excellent
energy-absorbing structures have been highly sought after
in engineering applications to improve devices and personal safety.
The ideal energy absorption mechanism should exhibit characteristics
such as lightweight, high energy absorption capacity, and efficient
reusability. To address this demand, a novel three-dimensional (3D)
chiral lattice structure with compression-twist coupling deformation
is fabricated by combining the left and right chiral units. The proposed
structure was fabricated in NiTi shape memory alloys (SMAs) by using
laser powder bed fusion technology. The compression experiment result
indicates that the shape recovery ratio is as high as 94% even when
the compression strain is over 80%. Additionally, the platform strain
reaches as high as 66%, offering high-level specific energy absorption,
i.e., 213.02 J/g. The obtained results are of great significance for
basic research and engineering applications of energy-absorbing structures
with high deformation recovery ratios